1 Liquid phase epitaxy using K₂W₂O₇ solvent produces high-quality Tm:KYW waveguide layers with thicknesses up to 40 µm and Tm concentrations from 0.7 to 1.2 at% at a growth rate of 18 µm/h.
“LPE is a well-known technique for the production of high-quality oxide films for laser applications, in which a single-crystal layer can be grown from a molten solution on a flat, oriented single-crystal substrate. 1-mm thick undoped KYW crystals with laser-grade polished (010) faces were used as substrates. The vertical dipping technique with partial immersion of the substrate was applied. Out of the two solvents employed recently for the fabrication of rare-earth-ion-doped KYW waveguides, a low-temperature chloride solvent [20] or K₂W₂O₇ [21], we chose the latter because of the much better interface and layer quality obtained with K₂W₂O₇ [19]. Single-crystalline layers with thickness up to 40 µm and different Tm 3+ concentrations ranging from 0.7 to 1.2at% were obtained at a growth rate of 18 µm/h”